Gold-VA-bath
Applications and
attributes
| One liter
bath |
| Gold-VA Concentrate
|
100 ml |
| Deionised water |
900 ml |
| Au-VA-replenisher (= 2 g Au) |
3,5 g |
Adjust the pH with electrometric equipment
or special, low pH paper in the range 0.2 to 0.6. The coating adhesion decreases
if the pH is too high.
Replenishing
Add 1.75 g Au-VA-replenisher per gram Au
removed from the bath. |
|
| |
Optimum |
Range |
| Au content |
2 g / l |
1 - 4 g / l |
| pH |
0.3 |
0.15 - 0.6 |
| Agitation |
> 5 m / min
(solution/mechanically) |
|
| Anodes |
PtNb (platinised
niobium)
MOXTi (mixed oxide coated titanium) |
|
| Current density |
4 A / dm² |
1 - 10 A /
dm² |
| Time |
6 min |
|
| Cathode
efficiency |
4.5 mg Au / A x
min |
|
|
|
|
| |
Deposit |
| Gold: |
AuCo-0,2% |
|
| Deposit density: |
17.5 g /cm³ |
|
| Hardness: |
approx. 160 VPN |
|
Please discuss your application with
us.
This